1. Panimula
Bronze casting is a foundational manufacturing process in modern industry, enabling the production of complex, high-performance components used in critical sectors such as marine engineering, pagbuo ng kapangyarihan, metalurhiya, transportasyon, at mabibigat na makinarya.
The process involves pouring molten bronze—an alloy primarily composed of copper and tin—into precision-designed molds to form parts that offer exceptional wear resistance, paglaban sa kaagnasan, mekanikal na lakas, at dimensional na katatagan.
From large centrifugal bushings and continuous-cast bearings to intricate impellers and pressure-retaining valve bodies, bronze castings provide reliable service under harsh operating conditions where ferrous alloys may corrode or fail.
The industrial value of bronze lies not only in its material properties but also in its adaptability to various casting methods, including sand casting, pamumuhunan paghahagis, sentripugal paghahagis, and continuous casting.
2. What Is Bronze Alloy?
tanso, as a class of copper-based alloys, is engineered by combining copper (Cu) with a range of alloying elements—most notably tin (Sn), but also including aluminum (Al), posporus (P), Silicon (Si Si), humantong sa (Pb), and others.
Each alloying addition modifies the base metal’s properties to meet specific industrial requirements such as strength, Paglaban sa Pagsusuot, paglaban sa kaagnasan, machinability, or thermal stability.

Composition and Alloy Types
| Uri ng haluang metal | Tipikal na komposisyon | Mga Pangunahing Katangian | Mga Karaniwang Aplikasyon |
| Tin tanso | Cu 88–92%, Sn 8–12% | Napakahusay na paglaban sa kaagnasan, mahusay na katatagan, katamtamang lakas | Marine components, mga bearing, mga gears, Mga balbula |
| Posporus tanso | Cu 90–95%, Sn 0.5–10%, P 0.01–0.35% | High fatigue resistance, springiness, magandang wear resistance | Springs, mga konektor ng kuryente, wear plates |
| Aluminyo Bronze | Cu 85–91%, Al 9–12%, Fe/Ni (traces) | Very high strength, outstanding corrosion and wear resistance (lalo na sa tubig dagat) | Mga propeller, Mga balbula, mga bahagi ng pump, aerospace fittings |
| Nanguna sa Tin Bronze | Cu 75–90%, Sn 5–12%, Pb 1–10% | Napakahusay na machinability, self-lubricating, good embeddability | Mga bearing, mga bushing, sliding components |
| Silikon tanso | Cu ~95%, Si 2–4%, sometimes Mn/Zn | Good weldability, katamtamang lakas, corrosion resistant | Hardware ng arkitektura, mga fastener, Mga aplikasyon ng marine |
| tanso ng mangganeso | Cu 55–65%, Zn 20–40%, Mn/Fe/Al (varied) | Mataas na lakas at katigasan, corrosion and impact resistance | Heavy-duty load-bearing parts, ship shafts, mga bahagi ng sasakyan |
| Nickel Aluminum Bronze | Cu ~80–85%, Al 8–11%, Ni 3–5% | Pambihirang paglaban sa kaagnasan, strength retention at high temperature | Offshore structures, naval components, petrochemical systems |
3. Why Choose Bronze Casting?
Superior Material Properties
- Paglaban sa kaagnasan: Bronze alloys exhibit excellent resistance to oxidation and corrosion, especially in marine, kemikal na, and atmospheric environments.
Aluminum and tin bronzes resist seawater corrosion and biofouling, making them ideal for marine hardware, mga bahagi ng pump, and valve systems. - Magsuot ng Paglaban at Tibay: Many bronze alloys, such as aluminum bronzes, offer exceptional hardness and abrasion resistance,
outperforming many steels in demanding applications like bearings, mga bushing, and heavy-duty wear components. - Thermal katatagan: Bronze retains mechanical strength and dimensional stability over a wide temperature range, including elevated temperatures found in industrial machinery and engines.
- Lubricity: Leaded tin bronzes provide inherent lubricity, reducing friction and wear in bearing applications without requiring external lubrication.

Casting Process Advantages
- Complex Geometry and Precision: Bronze casting allows the production of intricate and complex shapes—including hollow sections, manipis na pader, and fine details—that are difficult or costly to achieve by machining or forging.
Investment casting or centrifugal casting methods offer high dimensional accuracy and superior surface finish. - Cost Efficiency for Medium to Large Production Runs: Compared to wrought or machined components, bronze casting reduces material waste and machining time, especially for parts requiring high volume or complex shapes.
- Material Tailorability: The alloy composition can be adjusted to meet specific mechanical and chemical performance requirements.
This flexibility enables engineers to select alloys that balance strength, paglaban sa kaagnasan, machinability, at gastos.
Mechanical Performance and Reliability
- Mataas na Ratio ng Lakas sa Timbang: Bronze alloys offer an advantageous strength-to-weight ratio, suitable for components subjected to high mechanical loads without excessive mass.
- Pagkapagod at Epekto ng Paglaban: Phosphor bronzes, sa partikular na, provide excellent fatigue resistance and elasticity, making them valuable for springs, mga konektor, and dynamic load-bearing parts.
- Good Casting Integrity: When properly cast, bronze alloys produce dense, defect-minimized components with reliable mechanical properties, reducing failure risk in critical applications.
Application-Specific Benefits
- Mga Aplikasyon sa Marine at Offshore: Aluminum and tin bronzes resist corrosion in saltwater and aggressive marine environments, extending service life of propellers, mga bomba, and ship fittings.
- Bearing and Wear Components: Self-lubricating bearing alloys reduce maintenance needs and increase machine uptime, critical in industrial and automotive sectors.
- Aesthetic and Architectural Use: Bronze’s attractive patina and ability to be cast into artistic shapes make it popular for decorative and heritage applications.
Pagpapanatili at Recyclability
- Recyclable Material: Bronze alloys are highly recyclable without significant loss of properties, supporting sustainability initiatives and reducing raw material costs.
- Long Service Life: Durable bronze castings reduce replacement frequency and material consumption over product lifecycle, enhancing resource efficiency.
4. Bronze Casting Methods
Bronze casting employs several established techniques, each with distinct workflows, tooling requirements, and suitability for different production volumes and component complexities.
Sand Casting Bronze
Paglalarawan:
Sand casting is a versatile, time-tested process wherein a mold cavity is formed by packing sand around a pattern of the desired shape.
The sand mold, bound with clay or chemical binders, is porous, allowing gases to escape during pouring.
Molten bronze is then poured into this cavity, solidifying to replicate the pattern.
Sand casting accommodates large and complex parts with varied wall thicknesses, though mold surfaces produce a relatively rough finish.
The process enables quick design changes by modifying or replacing the pattern, making it ideal for prototyping and low-to-medium volume runs.
Cooling rates vary, influencing microstructure and mechanical properties.

Mga kalamangan:
- Low tooling and setup cost
- Suitable for large and complex parts
- Flexible for low to medium production volumes
- Easy to modify mold designs for prototyping
Mga Limitasyon:
- Rougher surface finish compared to other methods
- Lower dimensional accuracy
- Longer cycle times for mold preparation and finishing
Mga Aplikasyon:
Hardware ng dagat, large pump housings, mga bahagi ng arkitektura, and artistic sculptures.
Bronze Investment Casting (Nawala ang wax)
Paglalarawan:
Pamumuhunan sa paghahagis, also known as lost wax casting, involves creating a detailed wax pattern that precisely matches the final component geometry.
This pattern is coated repeatedly with refractory ceramic slurry, which hardens into a robust mold. Ang waks ay natunaw, leaving a cavity into which molten bronze is poured.
This technique allows exceptional detail and tight tolerances, producing castings with excellent surface finish and minimal machining requirements.
Due to the complexity of mold creation and the careful handling of wax patterns, investment casting is well-suited for small to medium batch production where precision and surface quality are paramount.

Mga kalamangan:
- Exceptional dimensional accuracy and surface finish
- Ability to produce complex, manipis na pader, and intricate geometries
- Minimal machining required post-casting
- Suitable for both small and medium production runs
Mga Limitasyon:
- Higher tooling and processing costs compared to sand casting
- Size limitations for very large castings
- Longer lead time due to pattern and shell preparation
Mga Aplikasyon:
Precision valve components, mga bahagi ng aerospace, art castings, at mga konektor ng kuryente.
Bronze Centrifugal Casting
Paglalarawan:
Centrifugal casting leverages rotational force to shape molten bronze inside a spinning mold.
As the mold spins rapidly around its axis, centrifugal force pushes the molten metal outward, ensuring dense metal packing against the mold walls.
This dynamic reduces porosity and inclusions, improving mechanical properties and structural integrity.
The process is particularly effective for cylindrical or tubular components, where uniform wall thickness and fine grain structure are critical.
Control over rotational speed and pouring temperature is crucial to avoid defects such as segregation or incomplete filling.
Centrifugal casting is often used in conjunction with secondary machining to achieve final dimensions.
Mga kalamangan:
- Produces dense, defect-free castings with fine grain structure
- Excellent control over wall thickness and dimensional consistency
- Reduced shrinkage and porosity defects
- High mechanical performance in critical components
Mga Limitasyon:
- Limited to rotationally symmetric parts
- Equipment investment is higher than sand casting
Mga Aplikasyon:
Mga bearing, mga bushing, Mga manggas, and cylindrical pump parts.
Bronze Permanent Mold Casting
Paglalarawan:
Permanent mold casting employs reusable metal molds, typically fabricated from steel or cast iron, into which molten bronze is poured.
Unlike expendable molds in sand or investment casting, these permanent molds allow for rapid production cycles with consistent dimensional control and surface finish.
The process often includes gravity or low-pressure filling, and solidification occurs faster due to metal mold heat dissipation, which results in a finer grain structure.
Gayunpaman, mold design complexity is limited by the need for part ejection and durability of the tooling. Permanent mold casting suits medium to high volume production of geometrically simple parts.
Mga kalamangan:
- Improved surface finish and dimensional accuracy compared to sand casting
- Faster cycle times due to mold reuse
- Suitable for medium to high production volumes
Mga Limitasyon:
- Initial mold tooling costs are high
- Limited to simpler geometries due to mold design constraints
- Less flexible for design changes
Mga Aplikasyon:
Standardized fittings, small mechanical parts, and architectural hardware.
Bronze Continuous Casting (Strip or Rod Casting)
Paglalarawan:
Continuous casting is a semi-continuous process where molten bronze is solidified into a continuous semi-finished shape—such as rods, Mga Billet, or strips—that can later be cut and processed into finished components.
Molten metal is poured into a water-cooled mold, solidifying quickly as it moves through the casting machine.
This process emphasizes efficient material use, uniform chemical composition, and consistent mechanical properties.
Though continuous casting is not a net-shape process, it provides reliable stock material for downstream machining or forging operations.
It is widely adopted in large-scale production environments focused on standard bronze alloy products.
Mga kalamangan:
- Efficient production of uniform raw materials
- Minimal na materyal na basura
- Consistent microstructure and mechanical properties
Mga Limitasyon:
- Not a net-shape casting process; further machining is required
- Limited to simpler shapes
Mga Aplikasyon:
Stock materials for bearings, mga bushing, and precision-machined parts.
5. Mold Materials and Gating Systems
The quality and integrity of bronze castings heavily depend on the choice of mold materials and the design of gating systems.
These factors influence metal flow, pagpapatibay, defect formation, at sa huli, the mechanical properties and surface finish of the final component.
Mold Materials
Sand Molds
Sand molds remain the most common in bronze casting due to their adaptability and cost-effectiveness.
Karaniwan, silica sand bonded with clay or chemical binders such as phenolic resins or sodium silicate is used.
For casting high-aluminum bronzes or where superior surface finish and thermal stability are needed, specialty sands like zircon or chromite are preferred because of their higher refractory properties and thermal conductivity.
Foundries carefully adjust sand properties—permeability, grain size, moisture content, and strength—to optimize performance for the specific alloy.
Halimbawa na lang, aluminum bronzes require low moisture levels (3–6%) and coarser sand grains to minimize gas-related casting defects.
Core sands, which form internal cavities, often employ higher-strength mixtures and are coated with graphite or similar substances to facilitate core removal without damage during shakeout.
Ceramic Shells
Investment casting employs ceramic shell molds made from refractory materials such as silica or zircon flour bound with colloidal silica.
These shells provide excellent resistance to the high pouring temperatures of bronze alloys and allow for extremely fine surface detail and tight tolerances.
The ceramic mold’s thermal stability ensures consistent solidification behavior critical for thin-walled and complex geometries.
Metal Molds (Permanenteng amag paghahagis)
Permanenteng mga hulma, typically constructed from cast iron or steel, are reused repeatedly for medium to high volume production.
Because bronzes tend to stick and chemically interact with iron at elevated temperatures, permanent mold casting is usually gravity-fed without the use of pressure to reduce mold-metal reaction and minimize iron pick-up in the casting.
Metal molds may be lubricated or preheated to extend mold life and improve casting quality.
Plaster and Other Specialty Molds
For very small, mataas na katumpakan na mga bahagi, plaster of Paris or ceramic-bonded molds are used, particularly in lost-foam or plaster casting processes.
These molds offer fine surface finish and dimensional accuracy but are limited to smaller batch sizes due to fragility and cost.
Gating Systems and Best Practices
An optimized gating system is fundamental for producing defect-free bronze castings.
It controls molten metal flow, minimizes turbulence, ensures proper feeding during solidification, and facilitates gas escape.
Gating Layout
Karaniwan, the runner—the horizontal channel conveying metal—is positioned in the lower half of the mold (drag), while gates (ingates) are placed in the top half (cope).
This arrangement allows the runner to fill first, trapping oxides and slag at the top of the metal stream where they can be more easily separated.
Wide, flat runners and gates help distribute molten metal evenly across the mold cavity and increase the surface area available for dross capture.
Direksyon ng Solidification
Gating and riser placement are designed to promote directional solidification—where metal solidifies first in the extremities of the casting and last in risers or feed reservoirs.
Techniques such as using a small choke (reduced gate area) encourage the molten metal to “heel” near risers, ensuring they remain the final point to freeze.
Chilled inserts or chills (metal blocks placed in thick sections) are often used to accelerate cooling in specific areas and direct solidification toward the risers, reducing shrinkage porosity risk.
Risers/Feeders
Risers serve as molten metal reservoirs to compensate for volume shrinkage during solidification.
Their size and placement are critical; a typical gating ratio by cross-sectional area is approximately 1:4:4 for sprue, runner, and gates respectively.
Use of insulated (mabuhay ka) risers or hot tops can improve feeding efficiency by maintaining molten metal temperature longer, preventing premature solidification.
Gate Design
Gates should be shaped to allow smooth, laminar metal flow into the mold cavity, minimizing turbulence that can cause gas entrapment and oxide formation.
Avoid sharp corners, abrupt cross-sectional changes, or bends in the gating channels.
Common design features include tapered sprues, gradual transitions, and radiused gates.
Fluxing the molten metal to remove oxides, combined with ceramic filters installed in gating systems, further reduces inclusions and impurities.
Pag-aayos ng Mga Salita
Molds must be effectively vented to allow trapped air and gases to escape during pouring.
This is achieved through vents—small slots or drilled holes placed at high points of the mold cavity—and through the inherent permeability of sand or porous mold materials.
Proper venting decreases defects such as blowholes and gas porosity.
Pouring Practices
Bronze should be poured at the lowest temperature sufficient to fill the mold completely, minimizing oxidation and dross formation.
Kinokontrol, steady pouring avoids splashing and turbulence. Advanced foundries may incorporate degassing treatments (hal., argon stirring) to further purify the melt and improve casting quality.
6. Mga Proseso Pagkatapos ng Paghahagis
The post-casting phase is essential to transform raw bronze castings into finished components that meet stringent mechanical, dimensional, at mga kinakailangan sa aesthetic.
This phase typically involves heat treatment, machining and finishing, followed by rigorous inspection and quality control.
Heat Treatment of Bronze Castings
Heat treatment plays a vital role in enhancing mechanical properties and relieving internal stresses induced during solidification and cooling.
- Stress-Relief Annealing: Most bronze castings undergo a stress-relief anneal, typically held between 300°C and 400°C, followed by slow cooling.
This process reduces residual thermal stresses, preventing distortion and cracking during machining and service. - Solution Treatment and Tempering (Mga tanso ng aluminyo): Aluminum bronzes are solution-treated at high temperatures (~1050°C) to dissolve precipitates and then rapidly quenched to form a martensitic α+β’ structure.
Subsequent tempering precipitates hard κ-phases, significantly increasing strength and hardness (hal., C954 aluminum bronze). - Annealing and Age Hardening (Phosphor Bronzes): Depending on requirements, phosphor bronzes may be annealed to improve ductility and machinability or age-hardened to enhance strength and fatigue resistance.
Machining and Finishing
Bronze castings typically require secondary machining to meet precise dimensional tolerances and surface finish specifications.
Common machining operations include turning, paggiling, pagbabarena, at paggiling.
The machinability of bronze alloys varies: leaded bearing bronzes and free-machining grades exhibit excellent chip control and lower cutting forces,
while aluminum bronzes—being harder and tougher—require more robust tooling and heavier cutting parameters.
Because bronze alloys are generally softer than steel but harder than brass, machining parameters are intermediate, balancing tool wear and surface quality. Post-machining finishing processes often include:
- Deburring and grinding: To remove casting flash, Mga Sprues, and any residual roughness.
- Shot blasting or sandblasting: To clean the surface and produce uniform texture, improving paint or coating adhesion.
- Polishing and plating: Polishing enhances aesthetic appeal and reduces friction, while plating (Chrome, nikel) provides additional corrosion and wear resistance, especially on pump shafts and moving parts.
Tin or zinc coatings are sometimes applied for corrosion protection in marine environments. - Patination: Used mainly for architectural or artistic castings, chemical patinas or wax coatings create desired color and surface effects.
Inspeksyon at Kontrol sa Kalidad (NDT)
Rigorous quality control is essential, especially for high-value or safety-critical bronze castings.
Finished parts undergo comprehensive dimensional inspection and non-destructive testing (NDT) to ensure integrity and compliance with design specifications.
- Radiographic Inspection (X-ray or CT scanning): Detects internal defects such as shrinkage cavities, gas porosity, and inclusions that could compromise mechanical performance.
- Ultrasonic pagsubok: Identifies subsurface cracks or voids not visible on the surface, providing high sensitivity for internal flaw detection.
- Visual and Dye-Penetrant Inspection: Used to locate surface-breaking defects like cracks, blowholes, or incomplete fusion areas.
- Pagsubok sa Katigasan: Confirms that the casting meets specified mechanical property targets after heat treatment.
- Chemical Analysis (Spectroscopy): Verifies alloy composition, ensuring material consistency and compliance with specifications.
7. Common Casting Defects and Their Prevention
Bronze castings can exhibit various defects if proper control measures are not implemented during the casting process.
Understanding the root causes and employing targeted prevention strategies are essential for producing high-quality castings. Key defects and their effective prevention methods include:
Gas Porosity
Gas porosity results from trapped gases within the casting, often caused by moisture in the mold sand, decomposition of binders, or air entrapment during pouring. This leads to voids or bubbles, weakening the casting’s integrity.
Prevention:
- Use dry, well-ventilated molds to facilitate gas escape.
- Minimize moisture content in the sand, as high moisture levels are particularly detrimental to copper-based alloys.
- Properly degas the molten bronze before pouring to reduce dissolved gases.
Shrinkage Cavities and Voids
Shrinkage cavities typically form in the last regions to solidify, often deep inside the casting, due to volume contraction as the metal cools.
Prevention:
- Design adequate risers and feeders to supply molten metal during solidification.
- Employ directional solidification by using chills or chill channels to control cooling from thinner to thicker sections.
- Optimize gating systems to ensure continuous feeding of molten metal into critical areas during solidification.
Sand and Slag Inclusions
These defects occur when sand grains or slag (dumi) become entrapped within the casting, compromising surface quality and mechanical properties.
Prevention:
- Use high-quality, low-friability sand and apply coatings on cores to prevent erosion during metal flow.
- Flux and skim the melt to remove slag and dross before pouring.
- Incorporate ceramic filters within the gating system to trap inclusions.
- Design gates to minimize turbulence and reduce the risk of sand wash-in.
Hot Tears and Cracks
Hot tears are cracks that develop while the casting is still semi-liquid or cooling, typically in long or slender sections, due to thermal stresses and restricted shrinkage.
Prevention:
- Improve mold collapsibility by incorporating parting planes or chills to relieve stresses.
- Use mold materials that allow some flexibility to accommodate shrinkage.
- Pour bronze at the lowest practical temperature to reduce thermal gradients and stresses.
- Control cooling rates to avoid rapid temperature changes that induce cracking.
Cold Shuts and Misruns
These defects occur when molten metal flow is insufficient or interrupted, causing incomplete fusion or unfilled sections.
Prevention:
- Increase pouring temperature and speed to maintain metal fluidity and flow.
- Improve gating system design to promote smooth, continuous filling of the mold.
- Reduce section thickness gradients to avoid flow stoppages.
- Preheat molds when necessary to maintain fluidity of the molten metal throughout the cavity.
8. Industrial Applications of Bronze Castings
Bronze casting occupies a vital role across numerous industrial sectors due to the alloy’s exceptional combination of mechanical strength, paglaban sa kaagnasan, Email Address *, at katatagan.

Marine and Offshore Industry
Bronze’s outstanding resistance to seawater corrosion and biofouling makes it a material of choice for marine components. Kabilang sa mga karaniwang application ang:
- Propellers and Pump Impellers: Aluminum and manganese bronzes provide strength and erosion resistance under harsh saltwater conditions.
- Valve Components and Seawater Fittings: Phosphor bronzes and tin bronzes resist corrosion and wear in control valves and piping systems.
- Ship Bearings and Bushings: Leaded bronzes offer excellent embedability and lubricity, ensuring reliable performance under heavy loads and misalignment.
Automotive at Transportasyon
Bronze castings contribute to critical components where durability and friction reduction are essential:
- Bushings and Bearings: Bearing bronzes provide low friction surfaces, extended wear life, and conformability, essential for suspension and drivetrain systems.
- Gear and Transmission Components: High-strength aluminum bronzes withstand impact and fatigue stresses.
- Mga Bahagi ng Sistema ng Preno: Phosphor bronze springs and clips offer resilience and fatigue resistance.
Aerospace
Sa aerospace, bronze alloys serve in applications demanding precision, lakas ng loob, at pagiging maaasahan:
- Valve Seats and Sleeves: Phosphor bronzes provide wear resistance in fuel and hydraulic systems.
- Mga konektor ng kuryente: Due to excellent conductivity and corrosion resistance, bronze alloys are widely used for connectors and terminals.
Industrial Machinery and Equipment
Bronze castings are integral in heavy machinery, where wear resistance and toughness are critical:
- Pump and Compressor Components: Mga Impeller, wear rings, and sleeves benefit from bronze’s hardness and corrosion resistance.
- Gear Wheels and Bearings: Aluminum and tin bronzes ensure long service life under cyclic loads.
- Valve Bodies and Fittings: Durable bronze castings withstand pressure and corrosive environments in chemical and power plants.
Mga Elektrikal at Elektronika
The excellent electrical and thermal conductivity of certain bronze alloys makes them suitable for:
- Switchgear and Relay Components: Phosphor bronze springs and contacts provide durability and corrosion resistance.
- Connectors and Terminals: Bronze alloys maintain reliable conductivity and mechanical strength under electrical cycling.
9. Pangwakas na Salita
Bronze casting remains a cornerstone of industrial manufacturing due to its unique combination of versatility, tibay ng katawan, at pagganap.
The broad spectrum of bronze alloys, each with tailored metallurgical properties, allows engineers and metalworkers to select compositions optimized for specific mechanical requirements, paglaban sa kaagnasan, and wear characteristics.
From traditional sand casting to advanced investment and permanent mold techniques, the casting methods offer flexibility in producing complex geometries with excellent surface quality and dimensional accuracy.
Sa kabuuan, bronze casting represents a mature yet continually evolving technology that bridges traditional craftsmanship with modern industrial needs,
making it an indispensable choice for engineers and manufacturers seeking materials that balance strength, paglaban sa kaagnasan, and manufacturability.
Mga FAQ
How does bronze casting differ from brass casting?
Bronze alloys primarily contain copper and tin (along with other elements), whereas brass alloys contain copper and zinc.
Bronze generally offers better corrosion resistance and wear properties, making it more suitable for heavy-duty and marine applications.
Are bronze castings suitable for high-temperature applications?
Bronze alloys maintain good mechanical properties at moderately elevated temperatures.
Aluminum bronzes, sa partikular na, retain strength and hardness after heat treatment, making them suitable for components exposed to heat and wear.
Is bronze magnetic?
Sa pangkalahatan, bronze is not magnetic because it is primarily a copper-based alloy. Gayunpaman, some bronze alloys with added ferromagnetic elements (like nickel or iron) may show slight magnetism.
Does bronze rust?
tanso does not rust because rust specifically refers to iron oxide forming on iron or steel.
Bronze can, gayunpaman, develop a greenish patina (oksihenasyon) over time when exposed to air and moisture, which actually protects the metal beneath.