1. Introduction
Heat treatment transforms aluminum castings from as‐cast, variable‐property components into precisely engineered parts that meet demanding application requirements.
By carefully controlling temperature, soak times, and cooling rates, foundries and metallurgists can tailor mechanical properties,
such as tensile strength, hardness, ductility, and fatigue resistance, while also improving wear characteristics, machinability, and dimensional stability.
This article delves into the fundamentals, processes, and best practices of heat treating aluminum castings.
We aim to provide a professional, authoritative, and comprehensive guide to engineers, metallurgists, and quality professionals seeking to optimize aluminum cast components for performance and cost.
2. Why Heat Treat Aluminum Castings?
The purpose of heat treatment is to:
- Increased Tensile Strength and Hardness
- Improved Ductility and Fatigue Resistance
- Enhanced Machinability and Wear Resistance
- Dimensional Stability and Residual‐Stress Relief
- Tailored Properties for Service Conditions
- Consistency and Quality Assurance

3. Common Aluminum Casting Alloys
Aluminum casting alloys are typically divided into two main categories:
- Sand casting / Permanent mold (gravity cast) alloys
- Die casting alloys (pressure cast)
They are designated by a four-digit number (e.g., A356, A319, A380) and fall into either the 2xx, 3xx, 4xx, or 7xx series depending on the primary alloying elements.
Table: Overview of Common Aluminum Casting Alloys
| Alloy | Primary Alloying Elements | Casting Process | Key Properties | Typical Applications |
|---|---|---|---|---|
| A356 | Silicon, Magnesium | Sand / Permanent Mold | High strength, good corrosion resistance, weldable | Aerospace, automotive wheels, marine parts |
| A319 | Silicon, Copper | Sand / Permanent Mold | Good machinability, moderate strength, good castability | Engine blocks, oil pans, transmission cases |
| A206 | Copper | Permanent Mold | Very high strength, low ductility, heat treatable | Aircraft fittings, structural parts |
| A380 | Silicon, Copper, Iron | High-Pressure Die Cast | Excellent castability, good strength, low cost | Housings, brackets, consumer electronics |
| ADC12 | Silicon, Copper, Iron | High-Pressure Die Cast | Good fluidity, wear resistance, dimensional stability | Automotive, electronics, small appliances |
| AlSi9Cu3 | Silicon, Copper | High-Pressure Die Cast | EU equivalent of A380; versatile and commonly used | Automotive gearbox housings, engine covers |
| 443.0 | Silicon, Magnesium | Sand / Permanent Mold | High corrosion resistance, moderate strength | Marine applications, pumps, valves |
| 535.0 | Magnesium | Sand / Permanent Mold | Excellent corrosion resistance, weldable | Marine hardware, architectural components |
4. What Types of Heat Treatment Are Available for Aluminum Castings?
The heat treatment process for aluminum castings varies based on the alloy composition, casting type, and desired mechanical properties.
Specialized furnaces and carefully controlled quenching methods are employed to ensure dimensional stability and prevent cracking during treatment. Below are common heat treatment types applied to aluminum castings:

TF (Fully Heat Treated)
The purpose of the TF treatment is to significantly increase the hardness and strength of aluminum castings.
The process involves heating the casting to around 515–535°C for 4 to 12 hours to dissolve alloying elements into a solid solution.
It is then rapidly quenched in warm water to prevent cracking, followed by aging at 150–160°C for 4 to 16 hours.
This treatment almost doubles the hardness of the original casting. TF is commonly used when high strength and durability are required, such as in structural components.
Its advantage lies in the substantial improvement in mechanical properties while maintaining casting integrity.
TB Condition (T4)
This heat treatment aims to improve ductility and moderate strength.
Castings are heated just below their melting point until alloy elements enter a solid solution, then quenched in water, boiling water, or polymer solution.
The quenching medium is selected to balance mechanical properties, reduce distortion, and minimize internal stress.
TB is suitable for parts that require good formability and weldability.
The advantage is the preservation of ductility and reasonable strength, which facilitates further manufacturing processes.
TB7 (Solution Treated and Stabilized)
Designed to produce castings with enhanced malleability, this treatment is similar to TF but with aging conducted at a higher temperature of 240–270°C for 2 to 4 hours.
This results in slightly softer castings compared to TF, making them easier to work with in applications where some flexibility is needed.
It’s used in components requiring better thermal stability and toughness.
TE (Age Hardening)
TE heat treatment accelerates the natural aging process by heating castings to 150–170°C for 4 to 12 hours without any quenching.
This is particularly useful for intricate or finely featured castings that could be damaged by rapid cooling.
The process improves hardness and stability without risking distortion. TE is preferred for delicate parts where shape retention is critical.
T5 (Precipitation Aging)
This artificial aging process stabilizes castings by heating them at relatively low temperatures (150–200°C) for 2 to 24 hours.
T5 improves machinability and dimensional stability and is typically applied to die castings where controlled hardness and surface finish are important.
The advantage is improved mechanical properties with minimal thermal impact on the casting.
T6 Temper
T6 treatment is used to achieve high strength and hardness.
The casting is solution treated at around 538°C for about 12 hours, rapidly quenched in water or glycol at 66–100°C, then artificially aged at 154°C for 3 to 5 hours.
Often, a straightening step follows quenching to ensure dimensional accuracy.
T6 is widely applied in aerospace, automotive, and defense industries for structural parts needing excellent mechanical performance.
Its main advantage is maximizing strength while minimizing deformation under load.
TF7 (T7 or T71 – Solution Treated and Stabilized)
This treatment enhances high-temperature mechanical stability by solution treating castings and stabilizing them at 200–250°C.
While it offers slightly lower tensile and yield strength than T6, TF7 improves thermal resistance and dimensional stability.
It’s ideal for components exposed to elevated temperatures or long-term stress.
Stress Relief and Annealing (TS Condition)
Stress relief heat treatment, performed at 200–250°C, reduces residual stresses that can cause warping or cracking.
Annealing, done at 300–400°C, softens castings for easier machining or forming.
These treatments are typically used for thick or complex castings requiring further mechanical operations. Their advantage is improved dimensional stability and enhanced workability.
Polymer Quenching
Instead of water, polymer solutions are used to quench castings at a slower rate.
This reduces internal stresses and distortion, making it suitable for complex or thin-walled castings that require less hardness but high dimensional accuracy.
Polymer quenching offers a gentler cooling method to protect delicate geometries.
Common Heat Treatment Types for Aluminum Castings Table
| Heat Treatment | Purpose | Process | Application | Advantages |
|---|---|---|---|---|
| T6 (Solution + Artificial Aging) | Maximize strength and hardness | Solution heat treatment (~530°C) → Rapid quenching → Artificial aging at 150–180°C | Automotive parts, aerospace structures, high-strength industrial castings | Excellent mechanical properties, high strength, good corrosion resistance |
| T5 (Direct Aging) | Quick hardening with low cost | Cast and then artificially aged at 160–200°C without solution treatment | Die castings (e.g., A380, ADC12) | Economical, simple process, improves surface hardness |
T4 (Natural Aging) |
Maintain ductility and moderate strength | Solution heat treatment → Quenching → Natural aging at room temperature for 96+ hours | Welded or formed parts | Good ductility, suitable for forming and welding |
| T7 (Overaging) | Enhance thermal and dimensional stability | Solution treatment → Aging at 190–220°C for extended time | High-temperature aerospace parts, precision components | Improved creep resistance, dimensional stability |
O Temper (Annealing) |
Relieve stress, soften material | Heat to 300–400°C → Hold for several hours → Slow cooling | Thick-walled castings, weld-repaired components, parts for machining | Enhanced machinability, soft structure, improved toughness |
| Homogenization | Reduce segregation, improve microstructure | Long soak at ~500°C for 12–24 hrs → Controlled cooling | Large cast ingots, billets for machining | Improved consistency, better mechanical properties |
| Stress Relieving | Reduce internal stress and warpage | Heat to 250–300°C → Hold for several hours → Air cooling | Precision parts, components after machining or welding | Improves dimensional stability, lowers cracking risk |
5. Alloy-Specific Heat Treatment Recipes
A356/356.0: Standard T6 Process
- Solutionizing: 540–560 °C, 6 h (25 mm section).
- Quench: Water (~20 °C) with mild agitation.
- Aging (T6): 160–165 °C, 6 h; air cool to ambient.
- Optional T7: 180 °C, 10 h; air cool.
A380/A383: T4 and T5 Applications
- T4 (Natural Aging): Quench from 505–525 °C; hold 18–24 h; limited strength (~UTS 200 MPa) with good ductility (4–6%).
- T5: Direct artificial aging at 160 °C for 4–6 h; results ~UTS 210–230 MPa, elongation 3–4%.

319/319.0: SHT and Aging for HPDC
- SHT: 505–525 °C for 4–6 h (10–20 mm sections).
- Quench: Polymer (10% PAG) to reduce distortion.
- Age (T6): 160–170 °C for 8–10 h; yields UTS ~260 MPa, elongation ~4–5%.
A413: High-Strength Castings
- SHT: 540–560 °C for 8–10 h (thick sections 50–100 mm).
- Quench: Water + corrosion inhibitor; aim for 400 °C/s cooling.
- Age (T6): 160–170 °C, 10 h; UTS ~270–310 MPa, elongation ~3–4%.
- Overage (T7): 180–200 °C, 10–12 h; UTS ~260–290 MPa, elongation ~5–6%.
6061 (Cast Variants) and Specialty Alloys
- 6061‐Cast SHT: 530–550 °C for 4–6 h (12–25 mm sections).
- Quench: Water or polymer (both acceptable for moderate distortion).
- Age (T6): 160 °C, 8 h; yields ~UTS 240–270 MPa, elongation ~8–10%.
- 6063‐Cast: Similar SHT, T5 often sufficient for UTS 165–200 MPa but T6 yields UTS ~210 MPa.
6. Mechanical Property Correlations
Tensile Strength, Yield Strength, and Elongation Post‐Treatment
- A356 T6: UTS 240–280 MPa; YS 200–240 MPa; Elongation 6–8%.
- A380 T5: UTS 210–230 MPa; YS 160–180 MPa; Elongation 3–4%.
- 319 T6: UTS 260–280 MPa; YS 210–230 MPa; Elongation 4–5%.
- A413 T6: UTS 270–310 MPa; YS 220–260 MPa; Elongation 3–4%.
Hardness Changes Through Heat Treatment Stages
- A356: As‐cast ~70 HB; after SHT ~60 HB; T6 ~80–85 HB; T7 ~75–80 HB.
- 319: As‐cast ~75 HB; T5 ~85 HB; T6 ~90–95 HB.
- A413: As‐cast ~80 HB; T6 ~95–105 HB; T7 ~90–100 HB.
Fatigue Performance and Crack Growth Rates
- A356 T6: Endurance limit ~70 MPa; T0 ~50 MPa.
- 319 T6: ~75 MPa; better high‐temp fatigue resistance due to finer Cu‐rich precipitates.
- Residual Stress Impact: Proper stress relief can boost fatigue life by 20–30%.
Creep Resistance in High‐Temperature Casting Applications
- Overaged A356 T7: Maintains ~85% of room‐temperature strength at 150 °C; acceptable for engine brackets.
- A413: T7 retains ~80% at 200 °C; recommended for transmission housings under sustained loads.
7. Applications of Aluminum Castings
Automotive Industry
- Engine Blocks (A356 T6): Demonstrated 20% weight reduction vs. cast iron; heat treatment yields UTS ~260 MPa, enabling higher cylinder pressures.
- Cylinder Heads (319 T6): T6 treatment eliminates porosity‐related fatigue failures; repeated runs across line yield consistent performance with <1% scrap due to quench cracking.

Aerospace Components
- Turbine Impellers (6061 T6): Through rigorous SHT and aging, achieve fatigue life >10⁷ cycles under 200 MPa stress; CMM post‐treatment confirms run‐out <0.01 mm.
- Landing Gear Blocks (A356 T7): Overaged for stability, retain 75% of strength at 120 °C; no in‐service cracking over 15,000 cycles in evaluation.
Industrial Machinery
- Pump Housings (A413 T6): T6 ensures UTS >280 MPa, reducing wall thickness by 20% vs. as‐cast designs; lubrication passages remain within ±0.05 mm after quench.
- Valve Bodies (A380 T5): Achieve UTS ~220 MPa, elongation ~4%; stress relief at 300 °C eliminates 80% of as‐cast distortion, reducing machining time by 30%.
Consumer Electronics and Heat Sinks
- Heat Sinks (6061 T6): Yield UTS ~250 MPa and thermal conductivity ~180 W/m·K; extruded and then heat‐treated for optimal performance in high‐power LED modules.
- Laptop Chassis (A356 T6): T6 ensures structural stiffness under mechanical loads; minimal warpage (<0.2 mm across 200 mm span) preserves panel fit and finish.
8. Conclusion
Heat treatment of aluminum castings is not a “one‐size‐fits‐all” proposition.
By understanding the metallurgical fundamentals—solutionizing, quenching, and aging—metallurgists can design cycles that optimize properties for specific alloys (6061, 7075, 356, etc.) and part geometries.
Through careful control of furnace temperatures, quench media, and aging profiles, castings transform into high‐performance components suitable for aerospace spars, marine hardware, automotive assemblies, and precision electronic enclosures.
Ultimately, successful heat treatment depends on:
- Alloy selection and chemistry
- Precise process control (temperature, time, quench rate)
- Post‐treatment inspection (NDT, mechanical testing, dimensional checks)
- Application‐driven temper choices (T6 for strength, T7 for stability, TS for stress relief)
By adhering to these principles and leveraging advanced furnace technology and metrologies, fabricators ensure that aluminum castings not only meet but exceed the mechanical, durability, and reliability standards of modern industries.